What are the inspection items for welding procedure qualification of flange prefabrication?
The main inspection items for welding procedure qualification are:
1.Weld visual inspection
The excess height of the weld metal shall not be lower than the base metal, the depth and length of the undercut shall not exceed the standard, and the weld surface shall be free of cracks, lack of fusion, slag inclusions, arc craters and pores.
2.NDT inspection of welds
The radiographic inspection of tubular specimens shall be carried out in accordance with the provisions of DL/T821, and the quality of the welds shall not be lower than the Class II standard. Non-destructive testing is not related to the mechanical properties of welded joints, but it is necessary to understand the state of welding defects in the "assessment". At the same time, it is also considered that it should be avoided when cutting the test piece. Therefore, it is included in the inspection items. It should be. The main purpose of fracture inspection is to check the macroscopic welding defects of the weld metal section, which belongs to the measurement range of the welder's operating skills and cannot be directly used to measure the mechanical properties, so it is cancelled.
Welding Procedure Qualification
Tensile Test (Dimensional Specimen)
① The excess height of the specimen shall be removed mechanically and shall be flush with the base metal.
② Thickness of the test piece: when the thickness is less than 30mm, the full-thickness test piece can be used, and when the thickness is greater than 30mm, it can be processed into two or more pieces of samples.
③ The tensile strength of each sample shall not be lower than the lower limit of the base metal.
④ The tensile strength of the dissimilar steel sample shall not be lower than the lower limit of the base metal on the lower side.
⑤ Two or more samples shall be subjected to tensile test, and the average value of each group of samples shall not exceed the lower limit of the specified value of the base metal.
Bending test
① Bending specimens can be divided into transverse face bends (back), longitudinal face bends (back), and lateral side bends.
② When T is less than 10, T=t; when T is greater than t, t=10. The width of the sample: 40, 20, 10 (unit: mm).
③ The excess height of the specimen shall be removed mechanically to keep the original surface of the base metal, and the undercut and the weld root notch shall not be removed.
④ If there is a defect on the lateral side bending surface, the more serious side shall be the tensile surface.
⑤ The three main factors that affect the bending test are: the ratio of the width to the thickness of the specimen, the bending angle and the diameter of the bending axis.
The bending test method and related regulations of SD340-89 regulations do not correspond to the elongation of the material itself.
Therefore, the elongation of the outer surface of the sample bending has exceeded the lower limit of the elongation for some steels, so it is not reasonable. .
In order to make the bending test more reasonable for the plasticity determination, the new regulations make the following provisions: the bending test method is carried out according to the GB/T232 metal bending test method.
The bending test conditions are specified as follows: the thickness of the sample is less than or equal to 10, and the diameter of the bending axis (D) is 4t. The distance between the supports (Lmm) is 6t+3, and the bending angle is 180 degrees.
For the steel whose lower limit of elongation is less than 20% specified in the standard and technical conditions, if the bending test fails and the measured elongation is less than 20%, it is allowed to increase the diameter of the bending shaft for the test.
On the tensile surface of the specimen, there shall be no cracking defects with a length of more than 3 mm in any direction in the weld and heat affected zone, except for cracks on the edges and corners, but cracks caused by slag inclusion defects shall be counted.
Impact test
As long as the pressure-bearing and load-bearing components meet the conditions for making impact test specimens, the impact test should be performed.
Therefore, it should be performed when the following conditions are met:
① If the thickness of the weldment is insufficient for sampling, it may not be performed.
② When the thickness of the weldment is ≥16mm, an impact test is required.
③ Evaluation qualification standard: The average value of the three samples should not be lower than the lower limit specified in the relevant technical documents, and one of them should not be lower than 70% of the specified value.
Metallographic inspection
For corner joints of tube sheets, the same incision shall not have two inspection surfaces.
Hardness test
The hardness of the weld and heat affected zone should not be lower than 90% of the hardness value, not exceeding the Brinell hardness of the base metal plus 100HB, and not exceeding the following requirements:
When the total alloy content is less than 3%, the hardness is less than or equal to 270HB; When the total content is equal to 3~10, the hardness is less than or equal to 300HB;
when the total alloy content is greater than 10, the hardness is less than or equal to 350HB P91 steel 220~240 is the best.